02 — Specifications: AISI 440C material parameters
These are the steel-grade parameters a stainless-bearing quotation
should be checked against — the ring and ball material is the spec
change a stainless bearing is actually bought for. Every value below is
transcribed from a collected source named in the row; no value is
rounded, averaged or added from memory. What is not here, by
registered omission (gap:02:partial-coverage): per-designation boundary
dimensions and load ratings — no collected record publishes them, and
they belong on the quotation against the maker's own table.
Chemical composition (AISI 440C, UNS S44004)
| Element | Content (wt%) | Source |
| Carbon (C) | 0.95 to 1.20 | aobosteel.com, published 2026-10-16 |
| Chromium (Cr) | 16.00 to 18.00 | aobosteel.com, published 2026-10-16 |
| Molybdenum (Mo) | 0.75 max | aobosteel.com, published 2026-10-16 |
| Manganese (Mn) | 1.00 max | aobosteel.com, published 2026-10-16 |
| Silicon (Si) | 1.00 max | aobosteel.com, published 2026-10-16 |
| Phosphorus (P) | 0.040 max | aobosteel.com, published 2026-10-16 |
| Sulfur (S) | 0.030 max | aobosteel.com, published 2026-10-16 |
The same ranges appear independently in the PatSnap corrosion analysis
(0.95–1.20% C, 16–18% Cr, published 2026-09-14) and its pitting
companion (Mn ≤1.0%, Si ≤1.0%, Mo ≤0.75%, P ≤0.04%, published
2026-09-14). Equivalent designations per aobosteel.com (2026-10-16):
AISI/SAE 440C / 51440C, UNS S44004, EN/DIN 1.4125, EN name X105CrMo17,
ASTM A276.
Mechanical properties and heat-treatment window
| Property | Annealed | Hardened & tempered | Source |
| Hardness | about 230 HB (270 HB max) | 57 to 60 HRC | aobosteel.com, 2026-10-16 |
| Tensile strength | about 758 MPa | about 1970 MPa | aobosteel.com, 2026-10-16 |
| Yield strength | about 430 to 450 MPa | about 1896 to 1900 MPa | aobosteel.com, 2026-10-16 |
| Elongation | 13 to 14% | about 2% | aobosteel.com, 2026-10-16 |
| Charpy V-notch | not typically reported | 3 to 5 ft·lbf | aobosteel.com, 2026-10-16 |
Heat-treatment window per aobosteel.com (2026-10-16): austenitizing
1010 to 1065 °C (up to 1095 °C), air or oil quench, subzero treatment
about −75 °C or lower, tempering about 150 to 370 °C (typical 315 °C).
The PatSnap chloride analysis narrows the working temper for corrosion
duty: 175 to 200 °C for 1–2 hours is its recommended balance, because
tempering above 150 °C starts precipitating chromium carbides and
exposure beyond ~2 hours in the 150–350 °C band measurably degrades
chloride resistance (published 2026-09-14). In the hardened state the
~2% elongation is the number to respect: 440C carries load well but
does not redistribute it — overload failure is sudden, not gradual.
Corrosion benchmarks: what "stainless" is worth here
| Benchmark | 440C value | Reference point | Source |
| Pitting potential (Epit) | +250 to +400 mV vs SCE | 316L ≈ +600 mV under the same conditions; 316L ≈ 0.1 μA/cm² vs 440C's 0.5–2.0 μA/cm² | eureka.patsnap.com, 2026-09-14 (3.5 wt% NaCl, deaerated, pH 6.5, 25 °C, 60 HRC) |
| Corrosion rate implied by icorr | 5 to 20 μm/year | — | eureka.patsnap.com, 2026-09-14 |
| Crevice-corrosion initiation (seawater) | 10 to 30 °C (crevice gaps 0.025–0.5 mm most vulnerable) | 316L initiates at 50 to 80 °C | eureka.patsnap.com, 2026-09-14 |
| Coastal atmospheric rate | 5 to 15 μm/year (passivated, lightly oiled; surface rust in 6–12 months unpainted) | — | eureka.patsnap.com, 2026-09-14 (ISO 9223 C5-Marine) |
| Seawater immersion (ASTM G52, 25 °C, 1 yr) | 20 to 40 μm/year average; splash zones 50 to 100 μm/year | duplex 2205 <5 μm/year, negligible pitting | eureka.patsnap.com, 2026-09-14 |
| Sensitization range | 450 to 850 °C (slow cooling or prolonged exposure depletes grain-boundary chromium) | — | eureka.patsnap.com, 2026-09-14 |
| Hot chloride condensates / brines | service above 80 °C needs supplementary protection (coatings, inhibitors) | — | eureka.patsnap.com, 2026-09-14 |
| Corrosion-resistance score (solution-Cr equation) | 440C scores 12.5 | 440A 14.2, 420 13.0, threshold for "stainless" = 11, 52100 chrome steel scores 1.0 | aobosteel.com chart, 2026-10-15 (equation from Knife Engineering, L. Thomas) |
Two boundaries follow directly and are buyer-decisive. First, matrix
chromium: ~12 wt% in solution is the minimum for passive-film
stability, and 440C's carbides can pull regions below it — which is why
the same 16–18% bulk chromium that names it "stainless" still pits in
chloride media (eureka.patsnap.com, 2026-09-14). Second, sulfur:
sulfide inclusions (MnS) are preferred pit-initiation sites, with
sulfur above 0.010 wt% significantly increasing susceptibility — a
certificate check worth asking for on washdown duty
(eureka.patsnap.com, 2026-09-14). The grade's own property source is
blunter: do not use 440C in chloride-rich environments, aggressive
chemical media, or high-temperature corrosion — mild service only
(aobosteel.com, 2026-10-16). Where the medium is the aggressive part,
section 03(d) is the decision.